Title: 鐵-9.0鋁-31.2錳-1.6碳合金相變化
Phase Transformations in an Fe-9.0Al-31.2Mn-1.6C Alloy
Authors: 邱世冠
Shih Kuan Chiu
劉增豐
T. F. Liu
材料科學與工程學系
Keywords: 相變化 ;phase transformation
Issue Date: 1993
Abstract: 我們利用光學顯微鏡(OM),X光能量分析儀(EDS)以及穿透式電子顯微鏡(
TEM)等,研究鐵-9.0鋁-31.2錳-1.6碳合金之相變化。在淬火狀態下其顯微
結構為沃斯田鐵相+細微的κ'-相碳化物,此κ'-相碳化物是在淬火過程
中於沃斯田鐵基地內以節點分解(Spinodal Decomposition)變態形成。且
具有L'12的結構。這種現象從未被其他鐵鋁錳碳合金研究者發現過。當此
合金在550℃至850℃時效處理後,在淬火過程中於沃斯田鐵基地形成的細
微κ'-相碳化物會沿<100>方向成長。增加時效處理時間,在晶界產生γ
→γ+κ-相的分解反應。這些結果和其他學者所觀察的現象截然不同。
更值得注意的是,此合金經750℃或低於750℃作時效處理,κ-相碳化物
為 L'12結構,而在850℃作時效處理時為L12結構。在950℃作時效處理時
,在晶界可以看到一些粗大的κ-相碳化物並且在沃斯田鐵基地內有淬火
過程中經由節點分解(Spinodal Decomposition)變態產生的細微κ'-相碳
化物。這種現象從未被其他學者發現過。
Phase transformations in the Fe-9.0Al-31.2Mn-1.6C alloy have
been investigated by using optical microscopy (OM),
transmission electron microscopy (TEM) and energy-dispersive X-
ray (EDS).In as-quenched condition, the microstructure of the
alloy was austenite phase containing (Fe,Mn)3AlCx({SYMBOL 107
\f {SYMBOL 162 \f "Symbol"}-phase) carbides.The {SYMBOL 107
\f {SYMBOL 162 \f "Symbol"}carbide has an L{SYMBOL 162 \f
12-type structure, which was formed within the austenite matrix
during quenching by spinodal decomposition.This feature has
never been observed by other workers in various Fe-Al-Mn-C
alloys. When the alloy was aged at temperature ranging from 550
{SYMBOL 176 \f "Symbol"}C to 850{SYMBOL 176 \f "Symbol"}C,
fine {SYMBOL 107 \f "Symbol"}{SYMBOL 162 \f "Symbol"}-
carbides existing in the as-quenched austenite matrix grew
preferentially along <100> directions.Prolonged aging at the
same temperature range, a {SYMBOL 103 \f "Symbol"} {SYMBOL
174 \f "Symbol"} {SYMBOL 103 \f "Symbol"} + {SYMBOL 107 \f
"Symbol"}-phase reaction could be found on the austenite grain
boundaries is quite different from that observed by other
workers in the Fe-Al-Mn-C alloys.It is worthy to note that the
{SYMBOL 107 \f "Symbol"}-phase carbide has an L{SYMBOL 162 \f
"Symbol"}12-type structure at 750 {SYMBOL 176 \f "Symbol"}C or
below and an L12-type structure at 850{SYMBOL 176 \f "Symbol"
}C.When the alloy was aged at 950 {SYMBOL 176 \f "Symbol"}C,
some coarse {SYMBOL 107 \f "Symbol"} -phase carbides could be
observed on the grain boundaries. Furthermore,extremely fine
{SYMBOL 107 \f "Symbol"} {SYMBOL 162 \f "Symbol"} carbides
could also be found within the austenite matrix by spinodal
decomposition during quenching. This feature has never been
found by other workers.