Abstract
As an approach to increasing their reliability, we doped Ag solder bumps with Pd and Au alloys to enhance their creep resistance, which we characterized using a nanoindentation technique. The hardnesses of the pure Ag and the Ag solders doped with Pd:3%, Pd:5%, and Pd:2%-Au:3% were 0.6 +/- 0.1, 1.8 +/- 02, 2.8 +/- 03, and 3.1 +/- 0.5 GPa, respectively. Although the hardness of the Ag solder was enhanced significantly when it contained Pd:2%-Au:3%, it exhibited a lower creep exponent (n > 2). The mechanism of the thermal recovery of the sample appears to be associated with activation of dislocation sources-also the reason for the decrease in hardness. The compounds doped with Pd:2%-Au:3% displayed significantly greater bond strengths and creep exponents, whereas the Pd only compounds exhibited poorer reliability. (C) 2017 Elsevier Ltd. All rights reserved.